Bridging and overhang sag
Plastic printed over empty air sags, droops or curls instead of staying flat. This usually means the plastic isn't cooling fast enough, or the printer is moving too fast or printing too hot for it to set in place.
Fixes, in the order to try them:
- Set the part cooling fan to 100% for bridges and overhangs in the slicer's cooling settings.
- Lower the bridge speed, starting around 20 to 30 mm/s.
- Turn on the slicer's option to slow down for overhangs so steeper sections print more gently.
- Lower the nozzle temperature 5 to 10°C, staying inside the range on the filament label.
- Reduce bridge flow slightly, for example to 0.9, so the strands are thinner and cool faster.
- Try the slicer's thick bridges setting if long, thin bridges sag or snap.
- Reorient the model or add supports for overhangs past about 55 degrees and for long bridges.