Clogged nozzle
Little or no plastic comes out of the nozzle, or it comes out thin and curling to one side. Something is blocking the nozzle, often burnt residue, dust, or softened plastic jammed higher up.
Fixes, in the order to try them:
- Heat the nozzle to the top of the filament's temperature range and push filament through firmly by hand.
- Do a cold pull: push cleaning filament or PLA through the hot nozzle, let it cool to around 90°C, then pull it out firmly.
- Repeat cold pulls until the tip comes out clean and shaped like the inside of the nozzle.
- With the nozzle hot, carefully push a 0.4 mm cleaning needle up through the tip.
- After switching from ABS, PETG or another hot material, purge with the new filament at the old, higher temperature.
- Replace the nozzle, a cheap wear part, following your printer’s instructions, since some printers change nozzles hot and others cold.
- Never touch the hot nozzle with your fingers; use the printer's tools or pliers, and let it cool before other work.
- On Bowden printers, re-seat the tube firmly against the nozzle.