Drooping or curling overhangs
Parts of the print that lean out over empty space droop, look ragged underneath, or curl upward at the edges. Overhangs steeper than about 45 degrees have little underneath to rest on, so they need strong cooling, slower printing or supports.
Fixes, in the order to try them:
- Run the part cooling fan at 100 percent for PLA, and turn on the slicer's extra fan for overhangs if it has one
- Turn on the slicer's slow-down for overhangs, or start steep overhangs at about 10 to 30 mm/s
- Lower the nozzle temperature 5 to 10°C, staying inside the range on the filament label
- Try a smaller layer height such as 0.12 to 0.16 mm so each layer steps out less
- Rotate the model on the bed so the worst overhangs are less steep
- Add supports for anything steeper than about 50 to 60 degrees; tree supports use less plastic and come off easier
- Turn on z-hop, which lifts the nozzle on travel moves, if curled edges are getting hit
- In your own designs, swap flat overhangs for 45 degree chamfers, which print cleanly without supports