Stringing and oozing
Thin hairs or cobwebs appear between separate parts of the print because plastic leaks from the nozzle while it travels. It usually comes from wet filament, a nozzle that is too hot, or retraction (the extruder pulling filament back before a move) set too low.
Fixes, in the order to try them:
- Dry the filament first, usually 4 to 6 hours at 45 to 55°C for PLA, 60 to 65°C for PETG, or 50 to 55°C for TPU.
- Lower the nozzle temperature in 5°C steps while staying inside the range on the spool label.
- Raise retraction a little at a time, usually 0.5 to 1.5 mm for direct drive and 3 to 6 mm for Bowden.
- Run the retraction test in OrcaSlicer, or a stringing test model, to find the best value.
- Calibrate pressure advance (also called linear advance), which evens out pressure in the nozzle and cuts oozing at stops.
- Raise travel speed and turn on 'avoid crossing walls' so the nozzle travels inside the part where strings won't show.
- Turn on wipe, which drags the nozzle along the wall before it travels, if a few strings remain.
- Keep z-hop low or off, because lifting the nozzle on every travel can add strings.